广东11选5开奖信息360

  • <tr id='Dgmj3t'><strong id='Dgmj3t'></strong><small id='Dgmj3t'></small><button id='Dgmj3t'></button><li id='Dgmj3t'><noscript id='Dgmj3t'><big id='Dgmj3t'></big><dt id='Dgmj3t'></dt></noscript></li></tr><ol id='Dgmj3t'><option id='Dgmj3t'><table id='Dgmj3t'><blockquote id='Dgmj3t'><tbody id='Dgmj3t'></tbody></blockquote></table></option></ol><u id='Dgmj3t'></u><kbd id='Dgmj3t'><kbd id='Dgmj3t'></kbd></kbd>

    <code id='Dgmj3t'><strong id='Dgmj3t'></strong></code>

    <fieldset id='Dgmj3t'></fieldset>
          <span id='Dgmj3t'></span>

              <ins id='Dgmj3t'></ins>
              <acronym id='Dgmj3t'><em id='Dgmj3t'></em><td id='Dgmj3t'><div id='Dgmj3t'></div></td></acronym><address id='Dgmj3t'><big id='Dgmj3t'><big id='Dgmj3t'></big><legend id='Dgmj3t'></legend></big></address>

              <i id='Dgmj3t'><div id='Dgmj3t'><ins id='Dgmj3t'></ins></div></i>
              <i id='Dgmj3t'></i>
            1. <dl id='Dgmj3t'></dl>
              1. <blockquote id='Dgmj3t'><q id='Dgmj3t'><noscript id='Dgmj3t'></noscript><dt id='Dgmj3t'></dt></q></blockquote><noframes id='Dgmj3t'><i id='Dgmj3t'></i>

                镍基合金做金相怎么选择金相腐蚀剂?

                2018-12-24技术资料

                前篇回顾:304不锈钢管热处理硬度不理想的解决方法

                镍基合金做金相怎么选择金相腐蚀剂?

                刚接触镍基合金,求问?Haynes 230,Haynes 625,Haynes X750,Haynes N 制备金相时候 采用什么 腐蚀剂? 腐蚀剂配比? 腐蚀时间?看网上好多种说法? 有的说是HCl:HNO3=3:1.。不知道哪个正确?

                HF:HNO3=1:3应该没有问题吧!至于腐蚀时间需要自己摸索.

                以前用这个腐蚀液腐蚀过Ni60A合金涂层的试样!

                用这个配比腐蚀Ni60用了多长时间?腐蚀后在电镜下能观察到什么形貌? 近期做了Ni基WC的喷涂层,想通广东11选五推荐号码过腐蚀Ni60,观察涂层中WC硬质相的分布,不知此法是否可取?

                这个试样用这个腐蚀是完全可广东福利彩票36选7开奖结果以的!腐蚀时间的话,你自己摸索下就可以了。

                那您配置的腐蚀剂就是用的分析纯硝酸和分析纯HF按1:3的比例配置的吗?配置时有何注意事项吗?比如试剂加入顺序什么的?

                都是用的分析纯,配置的时候顺序是将HF加入到HNO3中,还有注意的是配合的这个腐蚀也不能用玻璃器皿盛放,得用塑料盛放!